Ribboning and patterning in yarn winding

Ribbons are the shiny bands that appear on a wound package at certain diameters. They are built into the way random winders work, and they can be controlled.

What ribboning looks like

On a cross wound package, each layer of yarn should cross the layer below at an angle, giving an open, even surface. A ribbon is a band where the yarn has been laid directly on top of earlier wraps, coil on coil, for many layers in a row.

You can see ribbons as raised, shiny bands or a diamond pattern on the surface, and you can feel them as hard ridges.

Why it happens

It comes down to the wind ratio: the number of turns the package makes during one complete traverse out and back.

On a random winder, the package is driven by surface contact with a drum. Surface speed and traverse speed are constant, so the wind angle stays the same. But as the package grows, it turns more slowly, so the wind ratio keeps falling.

Every time the wind ratio passes through a whole number, or a simple fraction such as a half or a third, the yarn returns to exactly the same place it was laid on the previous traverse. For as long as the package stays near that diameter, wraps stack on wraps. That is a ribbon.

Because the critical ratios are fixed by the geometry, ribbons form at the same diameters on every package. The worst ones are at whole number ratios, and they get further apart and more severe as the package gets bigger.

What ribbons cost you

  • Breaks in unwinding. Stacked wraps trap each other. At high unwinding speed the yarn plucks, tension spikes and the end breaks, or several wraps slough off together.
  • Uneven dyeing. A ribbon is much denser than the package around it. Dye liquor flows around it, leaving light bands.
  • Damaged yarn. In a ribbon the drum presses on a narrow ridge, which can flatten or abrade the yarn.
  • Edge faults. Ribbons near the reversal points push yarn over the package edge, giving stitches and cobwebs.

A package with a bad ribbon often runs perfectly until the unwinding point reaches that diameter, which is why the fault shows up downstream as a break problem that seems to come and go.

Ways to prevent it

Ribbon breaking on random winders

Most drum winders have an anti patterning system. The common types are:

  • Speed modulation. The drum speed is cycled up and down so the package slips slightly and never settles at a critical ratio.
  • Cradle lifting or pressure relief. The package is briefly lifted or unloaded from the drum as it passes a critical diameter.
  • Traverse modulation. On machines with a separate traverse, its speed is varied in a controlled pattern.

If a winder that used to be clean starts making ribbons, check that this system is still working and set correctly before anything else. They are often switched off, set too mild, or worn.

Precision winding

A precision winder drives the package directly and gears the traverse to it, so the wind ratio is fixed for the whole package. Choose a ratio that is not a whole number or simple fraction and ribbons cannot form.

The price is that the wind angle falls as the package grows. Large precision wound packages can become too dense on the outside, with a wind angle too shallow to be stable. That limits package diameter.

Step precision winding

Step precision runs at a fixed safe ratio for a while, then steps to the next safe ratio as the package grows. The wind angle stays within a narrow band and the critical ratios are jumped over. It gives the density control of precision winding and the stable angle of random winding, on a more complex machine.

Which method for which job

Method Wind angle Wind ratio Suits
Random Constant Falls as the package grows Staple yarns, robust general purpose packages
Precision Falls as the package grows Constant Filament, sewing thread, dense packages
Step precision Nearly constant Stepped Dye packages, high speed unwinding

A quick diagnosis

  1. Measure the diameter where the ribbon or the unwinding break occurs. If it is the same on every package, it is a wind ratio problem.
  2. Check the anti patterning system is on and working.
  3. Check for slip. A glazed drum, low cradle pressure or a sticky package holder changes the real wind ratio and can move or worsen ribbons.
  4. Check tension. High winding tension makes every ribbon harder.
  5. If the package is for dyeing or fast unwinding and the winder cannot make it clean, the answer may be a different winding method.

Paul can help with winding problems on any type of winder, including deciding whether an existing machine can make the package your customer needs.

Tell Paul what the machine is doing

Send the yarn, the machine and the problem. You will get a straight answer on whether it can be fixed on the equipment you have, and what it would take.